AWS ER5183 Aluminum Welding Waya Aluminum MIG walda sandar Tig Waya

Takaitaccen Bayani:

ER5183 ya dace da MIG waldi na aluminum magnesium gami cewa ana buƙatar ƙarfin ƙarfi mafi girma kuma idan tushen tushe ya kasance 5083 ko 5654 ƙarfin ƙarfi zai zama mafi girma.An yadu amfani da waldi aluminum magnesium gami Tsarin jiragen ruwa, teku dandamali, locomotives & karusai, motor motocin, kwantena, cryogenic tasoshin da sauransu.


Cikakken Bayani

Tags samfurin

ER5183 ya dace da MIG waldi na aluminum magnesium gami cewa ana buƙatar ƙarfin ƙarfi mafi girma kuma idan tushen tushe ya kasance 5083 ko 5654 ƙarfin ƙarfi zai zama mafi girma.An yadu amfani da waldi aluminum magnesium gami Tsarin jiragen ruwa, teku dandamali, locomotives & karusai, motor motocin, kwantena, cryogenic tasoshin da sauransu.Karfensa na weld yana da kyau juriya ga lalata brine.

Matsayin walda: F, HF, V

Nau'in Yanzu: DCEP

SANARWA:

Tsayawa kunshin waya a cikin kyakkyawan yanayi kafin waldawa.

Duka saman da za a yi walda da walda da waya dole ne a share ƙazantar gurbataccen mai, shafi na oxide, danshi da sauransu.

Don samun kyakkyawan bayyanar weld wajibi ne don preheat tushe karfe zuwa 100 ℃-200 ℃ kafin walda idan ta kauri ne 10mm ko fiye.

Yana da kyau a sanya faranti a ƙarƙashin yankin walda don yada karfen da ya narke don tabbatar da shiga cikin walƙiyar.

Dangane da waldi matsayi da kauri na tushe karfe daban-daban garkuwa gas kamata a zaba, kamar 100% Ar, 75% Ar + 25% Shi, 50% Ar + 50% Shi, da dai sauransu.

Sharuɗɗan walda da aka ambata a sama don tunani kawai kuma yana da kyau a yi cancantar aikin walda bisa ga aikin kafin sanya shi cikin walƙiya na yau da kullun.

ER5183 KYAUTATA KARFE (%):

SI FE CU MN MG CR ZN TI AI BE
Daidaitawa ≤0.40 ≤0.40 ≤0.10 0.50-10 4.3-52 0.05-0.5 ≤0.25 ≤0.15 Ma'auni ≤0.0003
Na al'ada 0.08 0.12 0.006 0.65 4.75 0.130 0.005 0.080 Ma'auni 0.0001

KAYAN KIRKI NA ARFE ARFAFA (AW):

KARFIN TENSILE RM (MPA) KARFIN KARFIN KYAUTA (MPA) LABARIN A4 (%)
Na al'ada 280 150 18

Girma & Nasihar Yanzu don MIG (DC+):

ALAMAR WAYA DIAMETER (MM) 1.2 1.6 2.0
Welding Current (A) 180-300 200-400 240-450
Welding Voltage (V) 18-28 20-20 22-34

MANYAN KYAU & SHAWARAR YANZU DOMIN TIG (DCń):

ALAMAR WAYA DIAMETER (MM) 1.6-2.5 2.5-4.0 4.0-5.0
Welding Current (A) 150-250 200-320 220-400

  • Na baya:
  • Na gaba: