AWS E9015-G Low Alloy Karfe Welding sanda Low hydrogen Welding Electrodes J607CrNiMo

Takaitaccen Bayani:

J607CrNiMo (AWS E9015-G) ƙananan lantarki ne na ƙarfe na ƙarfe tare da ƙaramin murfin sodium na hydrogen.


Cikakken Bayani

Tags samfurin

Low Alloy Karfe Welding Electrode

J607CrNiMo                                       

GB/T E6015-G

AWS E9015-G

 

Bayani: J607CrNiMo ƙaramin ƙarfe ƙarfe ne na ƙarfe tare da ƙaramin murfin sodium na hydrogen.Yi amfani da DCEP (tabbataccen lantarki na yanzu kai tsaye), kuma ana iya walda shi a duk wurare tare da gajeriyar aikin baka.sandar walda tana da zurfin shigar ciki, ƙarancin spatter da kyakkyawan aiki.Ƙarfin da aka ɗora yana da kyakkyawan filastik, ƙarancin zafin jiki da juriya.

Aikace-aikace: Ana amfani da waldi na ruwa samar da bututu kasa 350 °C a wutar lantarki tashoshin da kuma matsa lamba jirgin steels na daidai ƙarfin maki.Yana da kyau ashana da gida WB36CN1 (HD15Ni1MnMoNbCu) karfe, kuma ya dace da walda WB3 (15NiCuMoNb5) karfe.

 

Abubuwan sinadaran na weld karfe(%):

C

Mn

Si

Cr

Ni

Mo

S

P

≤0.10

1.00 ~ 1.60

≤0.50

0.14 ~ 0.35

0.60 ~ 1.20

0.15 ~ 0.50

≤0.015

≤0.015

 

Abubuwan kayan aikin walda:

Gwaji abu

Ƙarfin ƙarfi

Mpa

Ƙarfin bayarwa

Mpa

Tsawaitawa

%

Ƙimar tasiri (J)

-30 ℃

Garanti

620 ~ 720

≥500

≥20

≥47

 

Yadawa hydrogen abun ciki na ajiyan karfe: ≤5.0mL/100g (Mercury ko gas chromatography hanya)

Duban X-ray: I grade

 

Shawarwari na yanzu:

(mm) da

Diamita na sanda

3.2

4.0

5.0

(A)

Welding Current

100 ~ 140

140 ~ 18

190 ~ 230

 

Sanarwa:

1. Dole ne a gasa wutar lantarki don 1 hour a kusa da 350 ℃ kafin aikin walda;

2. Yana da mahimmanci don tsaftace tsatsa, sikelin mai, ruwa, da ƙazanta akan sassan walda kafin walda.